01 Incomplete Base Formation (Concave Foot)
Symptoms: Poor bottom contour, especially concave bottom corners. While this does not significantly affect filling, it impacts bottle stability.
Causes:
- Insufficient high‑pressure air.
- Low temperature in the bottom‑corner area.
- Too short high‑pressure blow time (or too long pre‑blow time).
- Pre‑blow air intake too late.
- Blocked vent holes in the bottom mold.
Solutions: - Ensure high‑pressure air supply reaches at least 28 BAR.
- Check the high‑pressure filter on the mold side for blockages.
- Inspect valve operation to ensure accurate stretching and positioning during pre‑blow and high‑pressure molding.
- Verify pre‑blow and high‑blow control components for correct settings and clear passages.
- Ensure pre‑blow air is not initiated too late and does not last too long; otherwise, high‑pressure blow time will be insufficient, and effective cooling time in the mold will be reduced.
- Clear vent holes in the bottom mold.
- Increase the heating percentage or add more lamps in the bottom‑corner area to raise temperature.
- Adjust heating based on actual bottle conditions (weight and thickness distribution); reduce temperature in thinner areas to allow material to flow toward the bottom corners.
02 Neck‑Ring Swelling (Thread Swelling)
Symptoms: Swelling in the thread area, extending from the neck to the anti‑gas groove. More severe in hot weather, often accompanied by a hissing or bursting sound of leaking high‑pressure air.
Causes:
- Excessive cooling‑water temperature in the heater.
- Inadequate cooling‑water flow in the heater.
- Incorrect position of the heater’s cooling plates.
- Poor ventilation in the heater.
- Improper height adjustment of the heater lamp racks.
- Excessive temperature in Zone 1.
Solutions: - Check the temperature and flow rate of the heater cooling water.
- Adjust cooling‑plate position to properly protect the thread area (distance: 1.5 mm from preform front/back; 2 mm above the preform support‑ring plane).
- Increase heater fan ventilation or open side doors to improve air circulation and heat dissipation.
- Reduce Zone 1 heating percentage or reduce the number of lamps.
- Redesign the cooling plate if it is not properly designed.
03 Bent Neck (Crooked Neck)
Symptoms: The neck is tilted or bent to one side. The support ring below the thread is deformed and not perpendicular to the bottle body center. This defect seriously affects filling and capping.
Causes:
- Mechanical issues.
- Excessive mold‑body temperature.
- Insufficient cooling‑water flow to the mold body.
- Uneven temperature on the two sides of the mold body.
- Excessive material accumulation in the bottle neck.
Solutions: - Ensure proper clearance (about 0.25 mm) between the support ring and the mold‑top groove; the preform must be fixed while still hot.
- Check mold‑body water flow (insufficient flow raises temperature) and temperature (cooling‑water temperature or mold‑temperature controller). Uneven flow or temperature on the two sides causes differential shrinkage after demolding, leading to neck bending.
- Align the blow nozzle with the mold.
- If the neck has too much material, increase the heating percentage or add more lamps in that zone.
04 Blue Bottom Line (“Hot Bottle”)
Symptoms: A pearlescent streak along the bottom cut‑line; the affected area is thinner than on good bottles.
Causes:
- Excessive pre‑blow pressure.
- Too slow stretching.
- Pre‑blow air intake too early.
Solutions: - Prevent premature bottle inflation during pre‑blow (often caused by a faulty pre‑blow solenoid valve allowing high‑pressure air leakage).
- Reduce pre‑blow air pressure.
- Check stretching‑cylinder control pressure; clean solenoid valves, replace worn seals or broken coils that cause air leakage.
- Eliminate mechanical resistance in the stretching system (worn or dirty cylinder seals, misaligned stretching guides, or worn linear bearings).
- Ensure smooth exhaust from the stretching cylinder (clean muffler and clear air lines).
- Adjust the pre‑blow air‑intake timing.
05 Bottom Cracking
Symptoms: Fine cracks appear in overly thick bottom areas, often passing through or near the injection point.
Causes:
- Mechanical reasons.
- Insufficient preform bottom temperature (especially for bottles with flat‑bottom molds).
Solutions: - Check clearance between the stretch rod and mold bottom (clearance should be about 2/3 of the preform bottom thickness).
- Inspect the stretch‑rod cushioning.
- Increase heating percentage or add lamps in the bottom zone (low preform bottom temperature causes cracks when the stretch rod pushes it; however, too high a temperature can cause convex bottom).
06 Damaged Neck Threads
Symptoms: Damage to the neck threads or unwanted stretching of the thread‑area vent grooves.
Causes:
- Mechanical issues (preforms are fed into the mold by a transfer arm gripper; misalignment can pinch the threads during pickup; the take‑out gripper can also damage threads).
- Poor alignment between blow nozzle and mold (spring‑loaded nozzles cannot correct large misalignment; the impact force at blow‑start can damage threads).
- Excessive temperature in the thread area (high temperature allows vent grooves to stretch and deform, often accompanied by support‑ring warping).
Solutions: - Precisely adjust the transfer‑arm gripper (synchronization with the main turret and heater, clearance between gripper and mold top surface: 1 mm for loading, 0.7 mm for unloading).
- Use a dedicated tool to align the blow nozzle with the mold.
- Adjust cooling‑plate distance to better protect the threads, improve ventilation, reduce Zone 1 heating percentage, reduce lamps in Zone 1, or raise the heater frame (see also solutions for “Neck‑Ring Swelling”).
07 Excessive Liquid‑Level Drop After Filling
Symptoms: PET containers should undergo minimal change after filling. Excessive change is called excessive creep.
Causes: Containers should be blown at the lowest possible temperature. Excessively high temperature produces bottles with no pearlescence but maximum biaxial stretching, resulting in insufficient strength to resist expansion after filling. High‑temperature bottles are prone to bursting after expansion.
Solutions: Normally, a slight pearlescent appearance should be visible at the end of the blow‑molding stage. Set heating temperatures correctly during startup to avoid over‑ or under‑heating.
08 Bursting
Symptoms: Cracking at the bottom or near the bottom transition zone where thickness changes.
Causes:
- Material not reaching its natural stretch limit during blowing, leading to radial change (creep) after filling and bottom cracking.
- Folds formed at the bottom bursting during or after filling.
- Bottom too thin or too thick.
- Low IV value causing bottle expansion and rupture after filling.
- External damage to the bottom transition zone after molding.
- Excessive alkali concentration in chain lubricant.
Solutions:
For causes 1‑3, refer to the earlier “Bottom Cracking” section for corrective measures.